» Molybdenum - Molybdenium

Molybdenium is certified against ASTM B 386 (Molybdenum and Molybdenum Alloy Plate, Sheet, Strip, and Foil) and ASTM B 387 (Molybdenum and Molybdenum Alloy Bar, Rod, and Wire)

Composition Molybdenum Softening Temperature Molybdän Molybden
Physical Data Molybdän Mechanical Data Molybdenum Molybdän Molybden Molybdän Chemical Data

» Composition

  360 361 363 364 365 366
C max 0.03 % max 0.01 % 0.01-0.03 % 0.01-0.04 % max 0.01 % max 0.03 %
O max 0.0015 % 0.007 % 0.003 % 0.03 % 0.0015 % 0.0025 %
N max 0.002 % 0.002 % 0.002 % 0.002 % 0.002 % 0.002 %
Fe max 0.01 % 0.01 % 0.01 % 0.01 % 0.01 % 0.01 %
Ni max 0.002 % 0.005 % 0.002 % 0.005 % 0.002 % 0.002 %
Si max 0.01 % 0.01 % 0.01 % 0.005 % 0.01 % 0.01 %
Ti --- --- 0.4 - 0.55 % 0.4 - 0.55 % --- ---
W --- --- --- --- ---

27 -33 %

Zr --- --- 0.06 - 0.12 % 0.06 - 0.12 % --- ---
Mo Rem Rem Rem Rem Rem Rem

» Softening Temperature

Type Degree F Degree C
360 1650 900
361 1650 900
363 2100 1150
364 2100 1150
365 1650 900
366 2000 1100

» Mechanical Data

Type Temper Diameter T/S min. [MPa] Y/S min. [MPa] Elongation [%] DPH V 10 Kg
360, 361, 365 SR 0.020 to 1.8 (0.51 to 3.18), incl 585 450 15 ---
  SR over 1.8 to 13.32 (3.18 to 10.32) 515 380 15 ---
  SR over 13.32 to 7.8 (10.32 to 22.2) 620 515 18 230 - 280
  SR over 7.8 to 11.8 (22.2 to 28.6) 585 480 15 225 - 270
  SR over 11.8 to 17.8 (28.6 to 47.6) 515 450 10 215 - 260
  SR over 17.8 to 27.8 (47.6 to 73.0) 480 415 10 210 - 250
  SR over 27.8 to 31.2 (73.0 to 88.9) 450 380 10 205 - 240
363, 364 SR 3.16 to 7.8 (4.76 to 22.2), incl 790 690 18 260 - 320
  SR over 7.8 to 11.8 (22.2 to 28.6) 760 655 15 250 - 310
  SR over 11.8 to 17.8 (28.6 to 47.6) 690 585 10 245 - 300
  SR over 17.8 to 27.8 (47.6 to 73.0) 620 550 10 240 - 290
  SR over 27.8 to 31.2 (73.0 to 88.9) 585 515 5 235 - 285
366 SR 3.16 to 7.8 (4.76 to 22.2), incl 655 550 5 240 - 300
  SR over 7.8 to 11.8 (22.2 to 28.6) 620 515 4 235 - 300
  SR over 11.8 to 17.8 (28.6 to 47.6) 585 480 3 230 - 290
  SR over 17.8 to 27.8 (47.6 to 73.0) 550 450 3 230 - 290
  SR over 27.8 to 31.2 (73.0 to 88.9) 515 415 2 225 - 290
360 RX Under 2 (50.8) 415 240 20 200 max
  RX 2 to 31.2 (50.8 to 88.9) 380 170 20 200 max
363, 364 RX Under 2 (50.8) 550 380 20 215 max
  RX 2 to 31.2 (50.8 to 88.9) 515 310 10 215 max

» Chemical Properties

Electrochemical Equivalent 0.8949g/amp-hr
Electron Work Function 4.6eV
Electronegativity (Pauling) 2.16
Heat of Fusion 32kJ/mol

» Physical Properties

Atomic Mass Average 95.94
Boiling Point 4885K 4612°C 8334°F
Coefficient of lineal thermal expansion 0.0000066cm/cm/°C (0°C)
Electrical Conductivity 0.187 106/cm ohm
Thermal Conductivity 1.38 W/cmK
Density @ 300K 10.22g/cc
Elastic Modulus Bulk: 230/GPa
Rigidity: 20/GPa
Youngs: 329/GPa
Melting Point 2890K 2617°C 4743°F
Specific Heat 0.25J/gK